UralInduktor · metallurgical equipment manufacturing and supply
We will call back within 10 minutes

Selection and use of a melting crucible

Selecting a crucible requires three groups of data: the metal and melting mode, the geometry of the product, and the furnace design. The nominal capacity helps to find the size range but does not confirm compatibility with a specific unit.

What to check before ordering

  • Metal or alloy grade, working temperature, melt weight, and holding time.
  • Crucible material, fluxes used, and melt purity requirements.
  • Outer dimensions, inner geometry, bottom shape, support, and installation clearances.
  • Heating method; for an induction furnace — the frequency, the inductor dimensions, and the requirements for the melting unit.

How to read the dimension tables

In the extended ranges of round crucibles, D denotes the outer diameter at the top, D1 — the inner diameter at the top, d — the outer diameter of the bottom, H — the overall height. For magnesite crucibles, Dout and Din — the outer and inner diameters, H — the height, h — the depth of the cavity. For oval crucibles, L, B, B1, and H are used. For graphite crucibles for gold and quartz casings, the designations Φ1, Φ2, Φ3, and H are used. The relevant diagram is placed next to each table.

The dimensions apply to the selected series. A model number alone is not enough: identical designations occur on products with different geometry and material composition. If the capacity in kilograms is not given in a separate column, it must not be derived from the number.

Acceptance and handling

On receipt, the packaging, the outer and inner surfaces, the bottom, and the protective coating are inspected. Cracks, chips, and coating damage are recorded before installation. The crucible is not rolled across the floor, dropped, or moved by striking it. For transport, a suitable cart or fixture with soft supporting surfaces is used.

Storage

The storage area must be dry and ventilated, protected from precipitation and from floor moisture. Crucibles are placed on a stable stand or pallet. The stacking method and whether stacking is allowed are determined for the specific shape and packaging. A damp product is not placed directly into a hot furnace.

Installation in a fuel-fired furnace

Before installation, the dryness and condition of the working space are checked, and foreign metal residues and deposits are removed. The support must match the bottom of the crucible and provide stable seating while allowing for the intended thermal expansion. The height of the support, the installation clearances, and the relative position of the burner and crucible are set according to the furnace design.

A crucible with a pouring spout must rest with its body and bottom on the elements intended for this purpose. The spout is not used as a load-bearing element. In a tilting unit, the crucible mounting, the position of the supports, and the freedom of thermal movement are checked separately.

Installation in an induction furnace

The dimensions and condition of the inductor, the position of the crucible relative to the coil turns, the bottom support, the insulation, and the cooling system are checked. Clearances and intermediate materials are selected according to the design of the melting unit. Recommendations for one installation must not be automatically transferred to a furnace of a different power or frequency.

Drying and first heating

A porous material can absorb moisture. Before first use and after getting damp, the crucible is prepared according to an agreed procedure. It specifies the drying conditions, the heating rate, the duration of the holds, and the procedure for moving to the operating mode for the specific material and furnace.

Readiness for charging must not be judged by the glow color alone, and power must not be assigned based on the outer dimensions. Rapid heating of a cold or damp crucible can cause cracking, delamination of the coating, and separation of the bottom. After a break, the condition of the crucible and the need for repeated preparation are checked again.

Heating in a fuel-fired furnace

The burner and gas flows must ensure uniform heating without persistent local overheating of the wall or bottom. The burner setting, the atmosphere composition, and the power are matched to the furnace design and the crucible material. Flame impingement on a single spot and contamination of the working space change the heating conditions.

Charging the metal

The charge must be dry and prepared according to the process procedure. It is loaded carefully, without striking the bottom and walls. Large pieces must not wedge across the body: when heated they expand and can split the crucible. Sharp edges must not damage the coating.

The sequence and size of additional charging are set taking into account the amount of melt and the operation of the furnace. A large portion of cold metal can sharply cool the bath. The permissible working charge is checked separately from the nominal capacity.

Fluxes and process additives

The melting process dictates the composition, dosage, and order in which additives are added. Before use, the compatibility of the reagent with the crucible material is checked. Excess flux and its local accumulation at the wall can accelerate corrosion. Additives are introduced with the intended tool, without damaging the body and the coating.

Gripping and removal

The tongs or gripper must match the shape, size, and total weight of the crucible with its contents. The force is distributed over the designated area of the body. The rim must not be squeezed with an unsuitable tool or used as a fulcrum for a lever. Before removal, the condition of the gripper and stability during movement are checked.

Slag removal and cleaning

Deposits impair heat transfer, can act chemically on the wall, and can create stresses on reheating. The cleaning frequency and temperature are defined by the procedure. A suitable tool is used, without impacts and without cutting away crucible material; hardened residues are not knocked out by force.

Shutdown and cooling

After operation, the crucible is emptied of melt and cleaned in the manner specified by the process. Remaining metal can expand on reheating and damage the body. A hot crucible is placed on a dry, heat-resistant support provided for the purpose, avoiding contact with moisture and rapid cooling.

In the event of an unplanned shutdown, the pouring location, the procedure for handling the melt, and the conditions for the subsequent restart are defined by the shop procedure. A damaged product is not returned to service without an assessment of its fitness.

Damage: signs and possible causes

Below are 27 cases of damage, with the signs and the location of the defects described. The table helps to organize the inspection and collect data; the same defect can have several causes. In the case of cracks, through-damage, or unacceptable wear, follow the procedure for safe shutdown and replacement.

Transverse cracks

Transverse cracks
Symptom and locationPossible causes and what to check
At the bottom, up to separation of the bottom partToo-rapid heating, impacts on the bottom, expansion of remaining metal, impact of the charge on the inner surface.
Approximately in the middle of the bodyUneven or unsuitable support; gripping too high and excessive tong force; uneven heating.
Under the pouring spoutJamming of the body in the support during expansion and cooling; a stand that does not match the shape of the bottom.

Longitudinal cracks

Longitudinal cracks
Symptom and locationPossible causes and what to check
On a new crucible, from the lower part of the bodyPlacing a cold crucible into a hot furnace, rapid heating of the bottom, or local overheating. Accompanying coating delamination is possible.
On a long-serving crucible, in the thin-wall zoneWear and reduced load-bearing capacity of the wall; additional mechanical load.
A single crack from the top edgeUneven rapid heating, using the rim as a fulcrum for a lever, impact, or an unsuitable grip.
Several parallel cracks from the top edgePressure of the lid on the crucible, oxidation of the upper part of the body, slag buildup at the rim.
On the side wall, not reaching the edgesOutward pressure from inside: for example, expansion of a jammed, wedge-shaped piece of charge.

Star-shaped cracks and breakouts

Star-shaped cracks and breakouts
Symptom and locationPossible causes and what to check
Star-shaped crack in the bottomThermal shock or rapid local heating of the lower part.
Star-shaped crack on the side wallInternal pressure from the charge; mechanical impact.
Large hole without general thinning of the wallImpact during charging or cleaning. The way the crucible is handled and the tool used should be checked.
Small through holeCrack development. A shutdown per the procedure and an inspection of the body are required.

Chemical and local destruction

Chemical and local destruction
Symptom and locationPossible causes and what to check
Corrosion at the melt levelAction of flux, oxides, and surface deposits on the wall.
Corrosion in several placesIncompatibility of reagents with the material, or direct contact of an additive with the wall.
Corrosion of the bottom and lower partEffect of ash and slag in a fuel-fired furnace, local overheating.
Depression on the outer surfacePenetration of additives into the material and chemical degradation in the hotter zone.

Other signs

Other signs
Symptom and locationPossible causes and what to check
Network of cracks on the surfaceLong service and accumulated damage; an assessment of the remaining life is required.
Increased melting timeImproper crucible preparation, deposits on the walls, wear; the furnace operation is also checked.
Delamination of the protective coatingMoisture absorption, placing a cold product into a hot furnace, or too rapid heating.
Bulging and cracking of the bottomForeign solid inclusions under the bottom and uneven seating on a rigid surface.
Bottom crack with a thick layer of residual metal or slagExpansion of solidified residues on subsequent heating.
Greenish tint of the surface and softeningEffect of molten copper or prolonged overheating; the temperature and the composition of the deposits are checked.
Separation of the lower part of a new crucibleRapid heating of a damp product.
Deformation of the bodyUneven thermal expansion due to local overheating or rapid temperature change.
Accelerated oxidationCoating damage, air ingress, an unsuitable atmosphere, and long holds in an unfavorable temperature range.
General thinning of the wallsWear. The crucible is withdrawn from service when the limit set for the product is reached.
Sudden failure during operationIncluding moisture entering with the charge. The cause is determined after a safe shutdown; restarting without inspection is not permitted.

Reorder data

Keep the series designation, the drawing, the dimensions, and the material information. For damage analysis, attach an overall view of the crucible, close-ups of the defects, and data on the metal and fluxes, the temperature, the first heating, and the service time.

Corundum (alundum) and magnesite crucibles

The corundum series of 100–950 ml contains 99% Al₂O₃: long-term operation at 1600–1650 °C, briefly around 1700 °C. For the magnesite series made of fused magnesia, a long-term mode of 1700–1800 °C is specified. These values cannot be used to set heating and cooling rates or to determine service life.

Laboratory ceramics based on Al₂O₃ are selected according to the sample composition, temperature, and atmosphere. Heating and cooling must correspond to the selected grade of material. Direct contact with a cold or damp support after heating can cause thermal shock.

The lid does not seal the crucible and does not replace a protective atmosphere. For an induction furnace, check where the heat is generated: in the metal charge or in a separate conductive heater. Corundum ceramics cannot be used as a direct replacement for a graphite heater.

Dimensions of corundum (alundum) crucibles with lids.

Request for selection

Select a crucible

Specify the series or dimensions of the crucible, the metal, the furnace and the quantity. You can attach a drawing or photos of the installed crucible.